304 is the most widely used stainless steel in the world. It’s an austenitic chromium-nickel steel with about 18% chromium and 8% nickel, which is why it’s also sold as “18/8”. It resists corrosion well in air, water and most foods, forms and welds easily, is non-magnetic when annealed, and costs less than the molybdenum grades such as 316. Its main weakness is chlorides: salt water, pool chemicals and de-icing salt can pit it. This guide covers its composition, properties, international equivalents, the 304L and 304H variants, typical uses, and where you should pick something else.
Quick answers
- What it is: 304 is an austenitic stainless steel with 17.5–19.5% chromium and 8–10.5% nickel, and no molybdenum.
- Other names: 304 is also known as UNS S30400, EN 1.4301, SUS304 and, in cookware and fasteners, 18/8 or A2.
- Strength: Annealed 304 has a minimum tensile strength of 515 MPa (75 ksi) and a minimum yield strength of 205 MPa (30 ksi).
- Magnetism: Annealed 304 is non-magnetic, but bending or cold working can make it slightly magnetic.
- Corrosion: 304 handles kitchens, indoor use and inland outdoor use well, but salt, chlorine and warm chloride solutions can pit it.
- 304L: 304L is the low-carbon version (0.03% max carbon) and is the safer choice for welded parts thicker than about 5 mm.
- Food safety: 304 is the standard grade for sinks, cookware, dairy, brewing and food-processing equipment.
304 stainless steel at a glance
| Property | 304 (annealed) |
|---|---|
| Family | Austenitic (300 series) |
| Main alloying elements | Chromium 17.5–19.5%, nickel 8.0–10.5% |
| Molybdenum | None (that’s the key difference from 316) |
| Tensile strength, min. | 515 MPa (75 ksi) |
| Yield strength (0.2% proof), min. | 205 MPa (30 ksi) |
| Elongation, min. | 40% in 50 mm |
| Hardness, max. | 92 HRB / 201 HB |
| Density | About 7.9–8.0 g/cm³ (0.285–0.289 lb/in³) |
| Melting range | About 1,400–1,450 °C (2,550–2,650 °F) |
| Magnetic? | No when annealed; slightly after cold working |
| Hardenable by heat treatment? | No, only by cold working |
| Weldability | Excellent (filler 308 / 308L) |
| Typical uses | Sinks, cookware, food and drink equipment, appliances, architectural trim, tanks, fasteners |
Composition and mechanical values are ASTM A240 limits for plate, sheet and strip. Bar, pipe and wire specifications have similar but not identical limits.

Chemical composition of 304, 304L and 304H
The “304” name comes from the old AISI numbering, where the 300 series covers chromium-nickel austenitic steels. The table shows the ASTM A240 limits for the three common versions (percent by weight, single values are maximums):
| Element | 304 | 304L | 304H |
|---|---|---|---|
| Carbon (C) | 0.07 | 0.030 | 0.04–0.10 |
| Chromium (Cr) | 17.5–19.5 | 17.5–19.5 | 18.0–20.0 |
| Nickel (Ni) | 8.0–10.5 | 8.0–12.0 | 8.0–10.5 |
| Manganese (Mn) | 2.0 | 2.0 | 2.0 |
| Silicon (Si) | 0.75 | 0.75 | 0.75 |
| Phosphorus (P) | 0.045 | 0.045 | 0.045 |
| Sulfur (S) | 0.030 | 0.030 | 0.030 |
| Nitrogen (N) | 0.10 | 0.10 | – |
| Iron (Fe) | Balance (roughly 66–74%) | ||
What each element does:
- Chromium forms the thin, self-repairing chromium-oxide passive layer that makes the steel “stainless”. See can stainless steel rust?
- Nickel keeps the steel in the austenitic structure at room temperature. That gives 304 its ductility, toughness, weldability and non-magnetic behaviour. Nickel is also the main reason 304 costs more than ferritic 430.
- Carbon is kept low because, during welding or slow cooling, it can combine with chromium at grain boundaries and leave the surrounding metal short of chromium. 304L limits carbon further to avoid this.
Mechanical and physical properties
| Property (annealed) | 304 | 304L |
|---|---|---|
| Tensile strength, min. | 515 MPa (75 ksi) | 485 MPa (70 ksi) |
| Yield strength, min. | 205 MPa (30 ksi) | 170 MPa (25 ksi) |
| Elongation in 50 mm, min. | 40% | 40% |
| Hardness, max. | 92 HRB / 201 HB | 92 HRB / 201 HB |
| Density | About 7,900 kg/m³ (often rounded to 8.0 g/cm³) | |
| Elastic modulus | 193 GPa (28 × 10⁶ psi) | |
| Thermal expansion, 0–100 °C | 17.2 µm/m·°C | |
| Thermal conductivity at 100 °C | 16.3 W/m·K | |
| Specific heat, 0–100 °C | 500 J/kg·K | |
| Electrical resistivity | 720 nΩ·m | |
A few practical consequences of these numbers:
- Cold working makes it much stronger. The minimum strengths above are for soft, annealed material. Cold-rolled tempers (such as ¼ hard to full hard) and cold-drawn wire are far stronger, but less ductile. Heat treatment can’t harden 304. More on this in stainless steel hardness.
- It conducts heat poorly. 304 conducts heat only about a tenth as well as aluminium, or less. That’s why good cookware puts an aluminium or copper core inside the 304. See how to choose stainless cookware.
- It expands more than carbon steel. 304 expands roughly 40–50% more than mild steel with the same temperature rise, which causes more distortion when welding.
- Weight: 1 mm of 304 sheet weighs about 7.9 kg per square metre. Use the stainless steel weight calculator for other sizes, or read more on stainless steel density.
304 equivalents: 1.4301, SUS304, 18/8 and A2
The same grade goes by different names in different standards. These are functionally similar, not always identical in every limit, so check the actual specification for critical work.
| System | 304 | 304L |
|---|---|---|
| AISI / ASTM | 304 | 304L |
| UNS | S30400 | S30403 |
| EN (Europe) number | 1.4301 | 1.4307 (also 1.4306) |
| EN name | X5CrNi18-10 | X2CrNi18-9 |
| JIS (Japan) | SUS304 | SUS304L |
| GB (China) | 06Cr19Ni10 | 022Cr19Ni10 |
| Swedish SS | 2332 | 2352 |
| Trade and consumer labels | “18/8”, “18/10” (cookware and cutlery); “A2” (stainless fasteners) | |
18/8 and 18/10 describe roughly 18% chromium with 8% or 10% nickel. Both fall within the 304 family, so 18/10 cutlery isn’t a different grade, just 304-type steel at the higher end of the nickel range. 18/0 means almost no nickel, usually a 430-type ferritic steel. See 316 vs 18-8 stainless steel.
A2 is the fastener class for 18/8-type austenitic steel, usually 304. A4 is the molybdenum version, usually 316. More on fasteners in stainless steel bolts and nuts.
304 vs 304L vs 304H
| 304 | 304L | 304H | |
|---|---|---|---|
| Carbon | ≤0.07% | ≤0.030% | 0.04–0.10% |
| Strength | Standard | Slightly lower minimums | Higher at high temperature |
| Best for | General use, thin welded parts | Heavy welded sections, parts that can’t be annealed after welding | Pressure parts and structures at about 500–800 °C |
| Corrosion resistance | Essentially the same in ordinary conditions | ||
When 304 is held in the range of about 425–860 °C (800–1,580 °F), chromium carbides can form at grain boundaries. This is called sensitization, and it can leave a band next to a weld open to corrosion. Thin sheet cools quickly enough that it’s rarely a problem. In thick sections (roughly 5 mm and up), 304L avoids it without post-weld annealing.
In practice, much plate, pipe and bar is now dual-certified 304/304L: it meets the low-carbon limit of 304L and the strength minimums of 304 at the same time. Full comparison in 304 vs 304L stainless steel.
Corrosion resistance: what 304 handles and what it doesn’t
| Environment | 304 performance |
|---|---|
| Indoors, kitchens, dry or humid air | ✅ Excellent |
| Fresh drinking water (cold) | ✅ Good up to roughly 200 mg/L chlorides |
| Most foods, milk, beer, wine | ✅ Excellent with normal cleaning |
| Inland outdoor (rural, urban) | ✅ Good; occasional rinsing keeps it bright |
| Nitric acid, many organic acids | ✅ Generally good |
| Warm water with chlorides | ⚠️ Chloride limit drops (about 150 mg/L at 60 °C) |
| Coastal air, road de-icing salt | ⚠️ Tea staining and pitting are likely; 316 is better |
| Pools, spas, bleach left on the surface | ⚠️ Pitting risk; see stainless steel and chlorine |
| Seawater immersion | ❌ Not suitable |
| Hot, stressed parts in chloride solutions (above about 60 °C) | ❌ Stress corrosion cracking risk |
| Hydrochloric acid, most sulfuric acid concentrations | ❌ Poor; see hydrochloric acid and sulfuric acid |
Most “rust” on 304 is either surface staining from iron particles (from steel wool, carbon-steel tools or grinding dust nearby) or chloride pitting. Iron contamination cleans off and the passive layer re-forms. Pitting is permanent. Details in will 304 stainless steel rust? and passivation of stainless steel.
Heat resistance
- Oxidation (scaling) limit: about 870 °C (1,600 °F) in intermittent service and 925 °C (1,700 °F) in continuous service.
- Sensitization range: 425–860 °C. Long service here can reduce later corrosion resistance in wet conditions; 304L avoids this.
- Low temperatures: 304 stays tough down to cryogenic temperatures, which is why it’s used for liquefied-gas equipment.
- Annealing: heat to 1,010–1,120 °C (about 1,850–2,050 °F) and cool rapidly.
For hotter service, heat-resisting grades such as 309, 310 or 253MA are used instead. See is stainless steel heat resistant?
Working with 304: forming, welding and machining
- Forming: 304 is very ductile and can be deep drawn without intermediate annealing. That’s why sinks, saucepans and bowls are made from it. It work-hardens quickly, so it needs more force than mild steel and springs back more.
- Welding: it welds well by TIG, MIG, stick and resistance welding. The usual filler is 308L (308 or 308L under some codes). Use 304L for thick sections. Clean the heat tint afterwards to restore corrosion resistance. See how to weld stainless steel and the weld color chart.
- Machining: 304 is gummy and work-hardens at the cutting edge. Use sharp tools, slow speeds, steady feeds and plenty of coolant. Don’t let the tool rub. Where a lot of machining is needed, free-machining 303 or “improved machinability” 304 bar is often used.
- Fasteners: 304 bolts and nuts can gall (seize) when tightened quickly or dry. An anti-seize compound and slower tightening help.
- Avoid cross-contamination: use stainless-only brushes, discs and tools, because carbon-steel particles leave rust spots.
Common uses of 304 stainless steel
| Area | Typical 304 products |
|---|---|
| Kitchen and home | Sinks, cookware bodies, cutlery (18/8, 18/10), work tables, splashbacks, appliance parts |
| Food and beverage | Dairy, brewing and winemaking tanks, processing equipment, food storage |
| Architecture | Panels, trim, handrails and fixings in inland locations |
| Industry | Chemical containers, heat exchangers, pipe and tube, woven mesh and screens |
| Hardware | Bolts, screws, nuts (A2), springs, wire |
| Cryogenic | Equipment for liquefied gases |
304 comes in more forms and finishes than any other grade: sheet in every common gauge, plate, pipe (see the 304 pipe pressure rating chart), bar, wire and mesh.
When to choose another grade
| If you need… | Consider | Why |
|---|---|---|
| Better resistance to salt, chlorides or pool chemicals | 316 / 316L | 2–3% molybdenum resists pitting much better. See 304 vs 316. |
| Lower cost for dry, indoor, decorative parts | 430 | No nickel, so cheaper, but magnetic and less corrosion resistant. See 430 vs 304. |
| Lots of machining | 303 | Added sulfur makes it free-machining, at the cost of corrosion resistance and weldability. |
| Heavy welded sections | 304L | Low carbon prevents sensitization next to welds. |
| Hardness or a sharp edge | 410, 420, 440C | Martensitic grades can be hardened by heat treatment. |
| Service above about 900 °C | 309, 310, 253MA | Better scaling resistance at high temperature. |
| Cheaper austenitic option | 201 | Manganese replaces part of the nickel; lower corrosion resistance. See 201 vs 304. |
For the full picture of every family, see stainless steel types and grades.
How to tell if something is really 304
- Check the paperwork. For sheet, plate, pipe and bar, the mill test certificate (MTC) lists the heat’s actual chemistry and strength. It’s the only reliable proof short of testing.
- Try a magnet. Annealed 304 attracts a magnet very weakly or not at all. A strong pull suggests a ferritic or martensitic grade such as 430 or 410. Bent edges and cold-worked parts of genuine 304 can attract slightly, so a magnet can rule things out but can’t prove 304. See which stainless steel is magnetic.
- Telling 304 from 316 or 201 needs a test. A molybdenum spot test separates 304 from 316. Nickel-low 201 looks the same as 304, so a chemical spot test or a handheld XRF analyzer is the dependable way to check.
Frequently asked questions
Is 304 stainless steel food safe?
Yes. 304 is the standard grade for sinks, cookware, cutlery, dairy, brewing and food-processing equipment. It’s durable, easy to clean and resists most foods. For very salty or acidic process conditions, 316 is often preferred. See is stainless steel non-toxic?
Does 304 stainless steel rust?
Not in normal indoor or inland use, but it isn’t rust-proof. Salt, chlorine bleach, warm chloride solutions and embedded iron particles can cause staining or pitting. Clean with mild detergent and rinse well. See how to clean stainless steel.
Is 304 stainless steel magnetic?
Annealed 304 is non-magnetic. Cold working, such as bending, rolling or deep drawing, turns some of the structure into martensite, so formed edges and corners can attract a magnet slightly. That doesn’t mean the steel is fake or of lower quality. See stainless steel and magnets.
Is 18/8 the same as 304?
Essentially, yes. “18/8” refers to about 18% chromium and 8% nickel, which is 304’s composition. It’s mostly used on cookware, cutlery and fasteners. 18/10 is also a 304-type steel with a little more nickel.
Which is better, 304 or 316?
316 is better only at resisting chlorides and some chemicals, thanks to its molybdenum. Strength, appearance and weldability are essentially the same. Use 304 indoors and inland, and 316 near the sea, around pools or in chemical settings. See 304 vs 316 stainless steel.
Can 304 stainless steel be hardened?
Not by heat treatment. Heating and quenching 304 only anneals (softens) it. It can be strengthened only by cold working, which is how high-strength 304 spring wire and hard-temper strip are made.
Can 304 be used outdoors?
Yes, in inland urban and rural locations, especially with a smooth finish and occasional rinsing. Within a few kilometres of the sea, near road salt or in polluted industrial air, 316 holds up much better.
Last updated: November 2026. Composition, mechanical and physical values follow ASTM A240 and producer datasheets for grade 304/304L/304H (Atlas Steels). Equivalents are functional comparisons, not contractual matches. Always check the governing specification and mill certificate for critical or pressure applications.
Sponsored