316 stainless steel is the standard “marine grade” stainless steel and the second most widely used stainless after 304. It’s an austenitic chromium-nickel steel with 16–18% chromium, 10–14% nickel and 2–3% molybdenum. The molybdenum is what sets it apart: it gives 316 much better resistance to salt, chlorides and many chemicals than 304, at a higher price. Like 304, it is non-magnetic when annealed, forms and welds easily, and is safe for food. This guide covers its composition, properties in US and metric units, international equivalents (1.4401, SUS316, A4), the 316L, 316H and 316Ti variants, where 316 is used, and the limits that “marine grade” doesn’t tell you.
Quick answers
- What it is: 316 is an austenitic stainless steel with 16–18% chromium, 10–14% nickel and 2–3% molybdenum.
- Other names: 316 is also known as UNS S31600, EN 1.4401, SUS316 and, for metric bolts and screws, class A4.
- Why molybdenum matters: The 2–3% molybdenum makes 316 far more resistant to pitting from salt, chlorine and de-icing chemicals than 304.
- Strength: Annealed 316 has a minimum tensile strength of 515 MPa (75 ksi) and a minimum yield strength of 205 MPa (30 ksi).
- Magnetism: Annealed 316 is non-magnetic, and heavy bending or cold working can make it only very slightly magnetic.
- Marine use: 316 is the usual choice for boat fittings and coastal railings, but it can still tea-stain or pit in warm seawater and tight crevices.
- 316L: 316L is the low-carbon version (0.03% max carbon) and is the safer choice for welded parts thicker than about 3/16 in (5 mm).
316 stainless steel at a glance
| Property | 316 (annealed) |
|---|---|
| Family | Austenitic (300 series) |
| Main alloying elements | Chromium 16–18%, nickel 10–14%, molybdenum 2–3% |
| Tensile strength, min. | 75 ksi (515 MPa) |
| Yield strength (0.2% offset), min. | 30 ksi (205 MPa) |
| Elongation, min. | 40% in 2 in (50 mm) |
| Hardness, max. | 95 HRB / 217 HB |
| Density | 0.289 lb/in³ (8.0 g/cm³) |
| Melting range | About 2,507–2,552 °F (1,375–1,400 °C) |
| Magnetic? | No when annealed; very slightly after heavy cold working |
| Hardenable by heat treatment? | No, only by cold working |
| Weldability | Excellent (filler 316L) |
| Typical uses | Boat fittings, coastal railings, pool hardware, food and pharmaceutical equipment, lab and chemical equipment, fasteners |
Strength, elongation and hardness are the minimums (or, for hardness, maximums) for sheet, strip and plate under ASTM A240. Bar, pipe and tube have their own specifications with similar but not always identical values.

Chemical composition of 316, 316L and 316H
All three share the same chromium, nickel and molybdenum ranges. They differ only in carbon, which controls weldability and high-temperature strength.
| Element (%) | 316 | 316L | 316H |
|---|---|---|---|
| Carbon (C) | 0.08 max | 0.030 max | 0.04–0.10 |
| Chromium (Cr) | 16.0–18.0 | 16.0–18.0 | 16.0–18.0 |
| Nickel (Ni) | 10.0–14.0 | 10.0–14.0 | 10.0–14.0 |
| Molybdenum (Mo) | 2.00–3.00 | 2.00–3.00 | 2.00–3.00 |
| Manganese (Mn) | 2.0 max | 2.0 max | 2.0 max |
| Silicon (Si) | 0.75 max | 0.75 max | 0.75 max |
| Phosphorus (P) | 0.045 max | 0.045 max | 0.045 max |
| Sulfur (S) | 0.030 max | 0.030 max | 0.030 max |
| Nitrogen (N) | 0.10 max | 0.10 max | — |
Limits per ASTM A240 for flat-rolled product. Iron makes up the balance, roughly two-thirds of the alloy.
A quick way to compare chloride resistance between grades is the pitting resistance equivalent number, PREN = %Cr + 3.3 × %Mo + 16 × %N. With typical values of about 17% chromium, 2.1% molybdenum and 0.04% nitrogen, 316 scores around 24, against roughly 18–20 for 304. Higher means better resistance to pitting in salty water. It’s a ranking tool, not a guarantee.
Mechanical and physical properties
Mechanical properties (annealed, ASTM A240 minimums)
| Property | 316 / 316H | 316L |
|---|---|---|
| Tensile strength, min. | 75 ksi (515 MPa) | 70 ksi (485 MPa) |
| Yield strength (0.2% offset), min. | 30 ksi (205 MPa) | 25 ksi (170 MPa) |
| Elongation in 2 in (50 mm), min. | 40% | 40% |
| Hardness, max. | 95 HRB / 217 HB | 95 HRB / 217 HB |
Real material usually tests above these minimums, and cold working (rolling, drawing, bending) raises strength a lot. Many suppliers stock dual-certified 316/316L, which meets the carbon limit of 316L and the strength minimums of 316 at the same time.
Physical properties (typical, annealed)
| Property | US units | Metric |
|---|---|---|
| Density | 0.289 lb/in³ | 8,000 kg/m³ (8.0 g/cm³) |
| Modulus of elasticity | 28.0 × 10⁶ psi | 193 GPa |
| Thermal expansion, 32–212 °F (0–100 °C) | 8.8 µin/in·°F | 15.9 µm/m·°C |
| Thermal expansion, 32–1000 °F (0–538 °C) | 9.7 µin/in·°F | 17.5 µm/m·°C |
| Thermal conductivity at 212 °F (100 °C) | 9.4 BTU/h·ft·°F | 16.3 W/m·K |
| Thermal conductivity at 932 °F (500 °C) | 12.4 BTU/h·ft·°F | 21.5 W/m·K |
| Specific heat, 32–212 °F | 0.12 BTU/lb·°F | 500 J/kg·K |
| Electrical resistivity | 29 µΩ·in | 740 nΩ·m (0.74 µΩ·m) |
| Melting range | 2,507–2,552 °F | 1,375–1,400 °C |
Because 316 has the same density as 304, the weight of a sheet or plate is the same for both grades. Use the stainless steel weight calculator or the stainless steel gauge chart for thickness and weight per square foot.
316 equivalents: 1.4401, SUS316, A4 and more
316 is sold under different names around the world. These are functional equivalents, not exact contractual matches, so check the governing standard when the order is critical.
| System | 316 | 316L |
|---|---|---|
| AISI / SAE (US) | 316 | 316L |
| UNS | S31600 | S31603 |
| European (EN) | 1.4401 (X5CrNiMo17-12-2) | 1.4404 (X2CrNiMo17-12-2) |
| Japan (JIS) | SUS316 | SUS316L |
| Sweden (SS) | 2347 | 2348 |
| Old British (BS) | 316S31 | 316S11 |
| Metric fasteners (ISO 3506) | Class A4 (for example A4-70, A4-80), typically made from 316 or 316L | |
A4 vs A2: in metric bolts, nuts and screws, A2 is the 304-type class and A4 is the molybdenum-bearing 316-type class. The number after the dash is the strength class: A4-70 has a minimum tensile strength of 700 MPa (about 100 ksi), A4-80 of 800 MPa (about 116 ksi). In inch fasteners, the same steel is simply sold as “316 stainless”. For how “18-8” fasteners compare, see 316 vs 18-8 stainless steel.
316 vs 316L vs 316H (and 316Ti)
| Variant | What’s different | Choose it for |
|---|---|---|
| 316 | Standard grade, carbon 0.08% max | General parts, thin welded sections, fasteners, fittings |
| 316L | Low carbon, 0.030% max; slightly lower strength minimums | Welded parts thicker than about 3/16–1/4 in (5–6 mm), tanks and pipework that must stay corrosion-resistant without annealing after welding |
| 316H | Controlled higher carbon, 0.04–0.10%, plus a grain-size requirement | Pressure and structural parts working above about 930 °F (500 °C) |
| 316Ti (EN 1.4571) | Titanium-stabilized | Service around 1,100–1,650 °F (600–900 °C) and heavy welded sections |
Why carbon matters: when ordinary 316 is welded in heavy sections, chromium carbides can form at the grain boundaries next to the weld (“sensitization”), leaving a narrow band that corrodes faster. 316L has too little carbon for this to matter, so heavy welded 316 needs a post-weld anneal while 316L doesn’t. In everyday corrosion there’s usually no difference between 316 and 316L. The full comparison is in 316 vs 316L stainless steel.
Corrosion resistance: what 316 handles and what it doesn’t
316 resists a wide range of atmospheres and chemicals better than 304, especially anything containing chlorides: salt spray, pool and spa water, de-icing salt, brines and many process chemicals. That’s why it’s the default choice near the coast. But “marine grade” is a nickname, not a promise.
| Environment | 316 performance |
|---|---|
| Indoors, kitchens, inland outdoor use | ✅ Excellent (304 is usually enough here) |
| Coastal air, salt spray, road de-icing salt | ✅ Good, with smooth finishes and regular rinsing |
| Pool and spa hardware | ⚠️ Usually good; rinse regularly, because chlorine and salt residues build up on surfaces that rain doesn’t wash |
| Drinking water | ✅ Resists pitting up to about 1,000 mg/L chlorides at room temperature, only a few hundred mg/L when hot (140 °F / 60 °C) |
| Cold seawater, regularly rinsed or fully exposed | ⚠️ Usable, but expect brown “tea staining”, worst on rough surfaces |
| Warm seawater, stagnant seawater, tight crevices (under washers, gaskets, barnacles) | ❌ Pitting and crevice corrosion are likely; use duplex 2205 or a higher-alloy grade |
| Hot chloride solutions above about 140 °F (60 °C) under stress | ❌ Risk of stress corrosion cracking |
The brown staining you see on boat rails and seaside balustrades is usually surface corrosion, not structural damage. It’s most common on rough or scratched finishes and in crevices where salty water sits. A smooth, polished finish, designs that drain, and rinsing with fresh water keep 316 looking good. For causes and fixes, see why stainless steel rusts.
Heat resistance
- Oxidation (scaling) resistance: good in intermittent service up to about 1,600 °F (870 °C) and continuous service up to about 1,700 °F (925 °C).
- The range to avoid: long service between about 800 and 1,580 °F (425–860 °C) can sensitize standard 316 and weaken its later corrosion resistance. 316L, 316Ti or 316H are better choices there, depending on the job.
- Cold: like all austenitic grades, 316 stays tough down to cryogenic temperatures.
- Annealing: solution-anneal at 1,850–2,050 °F (1,010–1,120 °C) and cool rapidly. 316 cannot be hardened by heat treatment.
Working with 316: forming, welding and machining
- Forming: 316 bends, rolls and deep-draws well. It work-hardens as it’s formed, so it needs more force than mild steel and springs back more.
- Welding: excellent with TIG, MIG, stick and laser. Use a 316L filler (ER316L wire or E316L electrodes) so the weld keeps the molybdenum and the low carbon. Clean and passivate welds that will see chlorides, because heat tint lowers corrosion resistance. See how to weld stainless steel.
- Machining: 316 is gummy and work-hardens, so use sharp tools, rigid setups, steady feeds and plenty of coolant. Improved-machinability 316 bar exists. If machinability matters more than corrosion resistance, see 303 vs 316.
- Threads and galling: 316 bolts and nuts can gall (cold-weld) when tightened fast or dry. Use an anti-seize compound, tighten slowly and avoid power-driving stainless-on-stainless threads.
- Cutting: plasma, laser, waterjet and abrasive methods all work; keep carbon-steel dust away from the surface.
Common uses of 316 stainless steel
| Area | Typical 316 / 316L parts | Why 316 |
|---|---|---|
| Marine | Deck cleats, rails, stanchions, hinges, chain, rigging fittings, fasteners | Salt spray and splash |
| Coastal architecture | Balustrades, cable railings, cladding, trim, outdoor showers | Salt-laden air |
| Food and beverage | Processing equipment for salty, briny or acidic foods, dairy and brewing lines | Chlorides and cleaning chemicals |
| Pharmaceutical and lab | Tanks, piping, benches, lab equipment | Clean surfaces, harsh cleaning agents |
| Chemical and water | Chemical containers, heat exchangers, filtration screens, water and wastewater parts | Broad chemical resistance |
| Medical and jewelry | Implant-grade 316LVM, watch cases, body jewelry | Corrosion resistance against body fluids and sweat |
| Home and kitchen | Premium cookware, water bottles, sinks near the coast, outdoor kitchens and grills | Resistance to salt and acidic food |
Medical grade: implants use a cleaner, vacuum-melted version called 316LVM, made to ASTM F138 (bar and wire for surgical implants). Ordinary 316 or 316L is not automatically implant grade, and “surgical steel” on a label is a marketing term that can mean several grades. See surgical steel vs stainless steel.
Common US product standards: sheet, strip and plate are usually ordered to ASTM A240, bar to ASTM A276 or A479, and pipe to ASTM A312. Sheet thicknesses and pipe sizes are covered in 316 stainless steel sheet thickness and 316 stainless steel pipe dimensions.
When to choose another grade
| If you need… | Consider | Why |
|---|---|---|
| Lower cost, indoor or inland use | 304 | Same strength and look, no molybdenum premium |
| Warm seawater, higher strength | Duplex 2205 | Much higher chloride resistance and about twice the yield strength |
| More chloride resistance, still austenitic | 317L or 904L | Higher alloy content for better resistance to chlorides |
| Easy machining | 303 | Added sulfur machines far better, but corrodes more easily |
| Hardness and edge retention | 410 or 420 | Martensitic grades can be hardened by heat treatment |
| Service around 1,100–1,650 °F (600–900 °C) | 316Ti or 321 | Stabilized against sensitization |
Not sure between 304 and 316? The side-by-side guide is 304 vs 316 stainless steel, and an overview of all families is in stainless steel types and grades. For sheet sizes and finishes, see the stainless steel sheet metal guide.
How to tell if something is really 316
- Check the paperwork. For sheet, plate, pipe and bar, the mill test certificate (MTC) shows the heat’s actual chemistry, including molybdenum. Look for Mo between 2.00 and 3.00%.
- Look for markings. Pipe and plate are usually stamped with the grade and specification (for example “A312 TP316L”). Metric bolts carry “A4” on the head.
- A magnet can rule things out, not in. Annealed 316 doesn’t attract a magnet. A strong pull points to a ferritic or martensitic grade. But 304 isn’t magnetic either, so a magnet can’t tell 304 from 316. See which stainless steel is magnetic.
- Test for molybdenum. A molybdenum spot-test kit or a handheld XRF analyzer is the dependable way to separate 316 from 304.
Frequently asked questions
Is 316 stainless steel magnetic?
No, not in the annealed condition. Its austenitic structure is non-magnetic. Heavy cold working (sharp bends, cut edges, drawn wire) can create a little magnetism, usually less than in 304 because 316’s higher nickel keeps the structure more stable.
Does 316 stainless steel rust?
It resists rust very well, better than 304, but it isn’t rust-proof. Warm seawater, salt trapped in crevices, rough finishes and iron contamination from steel tools can cause brown staining or pitting. Rinse salt off, keep surfaces smooth and clean, and see how to clean stainless steel.
Is 316 stainless steel food safe?
Yes. 316 is widely used for food processing, dairy, brewing and pharmaceutical equipment, and for premium cookware and bottles. It behaves like 304 with food, with extra resistance to salty and acidic foods and cleaning chemicals.
What is the difference between 316 and 316L?
316L has a lower carbon limit (0.030% vs 0.08%). That protects welded areas from sensitization, so 316L is preferred for welded parts thicker than about 3/16 in (5 mm). Otherwise they behave almost the same, and much stock is dual-certified to both.
Is 316 better than 304?
For salt, chlorides and chemicals, yes. For strength, looks, weldability and indoor use, they’re essentially equal, and 304 costs less. Choose 316 near the sea, around pools, near road salt and in chemical or medical settings.
What is the melting point of 316 stainless steel?
316 and 316L melt over a range of about 2,507–2,552 °F (1,375–1,400 °C), slightly lower than 304. Its useful service limit in air is far lower, about 1,600–1,700 °F (870–925 °C).
Is SUS316 the same as 316?
Yes. SUS316 is the Japanese (JIS) name for the same grade, and SUS316L matches 316L. Europe’s equivalents are 1.4401 and 1.4404.
Last updated: November 2026. Composition and mechanical values follow ASTM A240 limits as published in producer grade datasheets (Atlas Steels, via worldstainless); melting range from BSSA (ASM Specialty Handbook data). US-unit values are converted from the metric figures and rounded. Equivalents are functional comparisons, not contractual matches. Always check the governing specification and mill certificate for critical, pressure or implant applications.